Extrusion, Clearance and Back-Up Rings: When Hardness Is Not Enough

Extrusion starts where the clearance is wider than the rubber can bridge. How to check a joint against the pressure-clearance limit, and how a back-up ring changes the calculation.

10 min read 1,259 words Updated 2026-11-17

Extrusion is the failure that looks like wear and is not. The ring is not rubbed away by motion; it is forced into the gap between two metal parts by pressure, and sheared off at the edge. Once started it is progressive: the damaged edge leaks, the leak increases local pressure on the damage, and the ring fails completely.

Whether it starts is decided by three numbers, and only one of them is about the rubber.

The production floor
Extrusion is a clearance problem before it is a material problem.

The mechanism in one paragraph

Under pressure, an O-ring is pushed toward the low-pressure side of the gland until it touches the clearance gap. The rubber cannot flow like a liquid, but it creeps: at high stress and temperature it deforms into the gap. If the gap is wider than the rubber can bridge, the extruded tongue is cut off by the metal edge on the next pressure cycle. The result is a ring with a chewed, feathered or stepped edge on the low-pressure side, and a groove edge with a matching witness mark.

The three variables

Pressure. The driving force. Extrusion risk rises faster than pressure because the shear stress at the gap edge rises with it.

Clearance. The gap the rubber has to bridge. Usually a diametral clearance between bore and piston, or between a cover and its seat. It is determined by the tolerance stack, not by the nominal drawing.

Temperature and hardness. Hot rubber is softer rubber. A 70 Shore A compound at 100 °C is effectively softer than the same compound at 23 °C, so the pressure-clearance limit that applied on the test bench no longer applies in service.

The pressure–clearance limit

Published gland design guides give a ceiling for each hardness. The shape is what matters:

System pressureMax clearance, 70 Shore AMax clearance, 90 Shore A
1,000 psi0.012 in0.016 in
1,500 psi0.008 in0.012 in
2,000 psi0.005 in0.008 in
2,500 psi0.004 in0.006 in
3,000 psi0.003 in0.005 in
5,000 psiback-up ring requiredback-up ring required

Read the table as a design limit, not a test result. It is the clearance at which the ring is expected to survive continuous service at that pressure and moderate temperature, with a reasonable surface finish.

Two practical consequences:

  1. A 70A ring is a moderate-pressure seal. Above about 1,500 psi, the clearance needed to assemble a normal joint is already at or beyond the limit.
  2. The fix is not more squeeze. Adding squeeze increases the force pushing rubber into the gap. It shortens life and does not close the clearance.

What a back-up ring actually does

A back-up ring is a hard ring — usually PTFE, filled PTFE, PEEK or a 90 Shore A elastomer — placed on the low-pressure side of the O-ring. It does not seal; it blocks the gap. The O-ring then presses against a hard, flat face instead of trying to extrude into a clearance.

The effect on the pressure rating is large: a joint that would extrude at 2,000 psi with a 70A ring alone can run at 5,000 psi or more with a back-up ring, depending on the back-up material and the clearance.

Three design rules follow:

  • The back-up ring goes on the low-pressure side. In a double-acting system, that means two back-up rings, one on each side of the O-ring.
  • The groove must be wider. A back-up ring needs its own axial space — typically 0.03–0.06 in per ring for this size range — so the groove width increases and the fill calculation has to be redone.
  • The back-up ring has its own clearance limit. PTFE back-ups extrude too, just at a much higher pressure. A spiral failure of a back-up ring is common where the groove is too wide or the ring is installed with a twist.

Types, and when each is used

TypeShapeUse
Solid (flat)Rectangular sectionStandard static and dynamic joints; simplest groove
Contoured (V or concave)Matches the O-ring curvatureDynamic service; keeps the O-ring centred, less friction
SplitCut through one pointInstallation over a piston without dismantling; lower pressure rating
Elastomeric 90ARubber, not plasticModerate pressures where PTFE's creep is a problem

The military designators carry this through: for each dash number in the MS28775 and AS3209 families the standard lists a matching back-up ring, for example MS28774-214 for the 214 size. If your drawing calls for a military seal and a back-up, the part number pair is already defined — do not invent a PTFE ring of nominal dimensions, because the back-up ring section is not the O-ring section.

Where the design usually goes wrong

The groove width is not increased. The back-up ring is added to an existing groove, the fill ratio goes over 90 %, and the joint becomes hydraulically locked or the O-ring is pinched between the back-up and the groove wall.

One back-up in a double-acting cylinder. Pressure reverses, the unprotected side extrudes, and the failure looks like a material problem on the wrong face.

A split back-up installed with the gap aligned to the leak path. The split should face away from the pressure, and in a rotary application it should not sit in line with a port.

PTFE back-ups in a joint that cycles in temperature. PTFE creeps and has a high expansion coefficient; a back-up ring sized for 23 °C can be an interference fit at 120 °C.

The order of remedies for extrusion

is: reduce clearance, add a back-up ring, increase hardness. In that order. Reversing it — going to 90A first — raises seating load and cost while leaving the gap untouched.

Diagnosing extrusion on a failed part

Look at the low-pressure side of the ring. Extrusion leaves a feathered, chewed or stepped edge, sometimes with a piece missing. The groove edge on the same side will show a polished witness mark where the rubber was forced against it.

Distinguish it from installation damage: installation cuts are clean, cross the section, and appear where the ring passed an edge during assembly. Extrusion damage is on one side only, follows the circumference, and is accompanied by material displacement rather than removal.

Frequently asked questions

At what pressure do I need a back-up ring?

With a 70 Shore A ring and a normal machined clearance, around 1,500–2,000 psi is the practical ceiling. With 90 Shore A, around 2,500–3,000 psi. Above that, use a back-up ring regardless of hardness.

Can I use two back-up rings with one O-ring?

Yes, and in a double-acting cylinder you must — one on each side. The groove width has to be increased accordingly, and the fill ratio recalculated.

Does a back-up ring seal anything?

No. It blocks the clearance so the O-ring does not have to. The O-ring still does all the sealing, which is why a damaged back-up ring alone does not usually cause a leak until the O-ring follows it into the gap.

What material should a back-up ring be?

PTFE for most service, filled PTFE (glass, bronze, carbon) where creep or wear resistance matters, PEEK for high temperature and aggressive media, and 90 Shore A elastomer for moderate pressure where a plastic ring's creep is a problem.

Why did my back-up ring fail in a spiral?

Too much clearance behind it, a groove that is too wide, or installation twist. A back-up ring needs radial support as much as the O-ring does, and a split ring installed with the split in the wrong place will open under pressure.

Scope